Nd:YAG laser influence on tensile bond strength of self-etching adhesive systems
A B Matos1, D C Oliveira, R S Navarro
1University of São Paulo, School of Dentistry, Operative Dentistry Department, São Paulo, Brazil. bona@fo.usp.br
Objective:
We evaluated the tensile bond strength of composite resin on enamel and dentine, treated with Nd:YAG laser before and after bonding procedures.
Background Data:
The use of laser radiation in dentistry is being developed day by day. One of the possible applications of dental lasers includes increasing the quality of self-etching bonding systems.
Methods:
Forty-eight human teeth were used and separated into six groups: Group 1 (enamel control), Clearfil Liner Bond 2V (CLB 2V); group 2 (enamel), Nd:YAG + CLB 2V; group 3 (enamel), CLB 2V + Nd:YAG; group 4 (dentine control), CLB 2V; group 5 (dentine), Nd:YAG + CLB 2V; group 6 (dentine), CLB 2V + Nd:YAG. Tensile bond strength was performed.
Results:
Enamel means (15,54) were lower than dentine means (20,38). Bond strength of laser before (15,73) was lower than laser after (20,65). Interaction results G1 x G3; G2 x G3; G4 x G1; G2 x G5 were statistically significant.
Conclusions:
Tensile bond strength of composites reached with self-etching adhesive systems were greater in dentine than in enamel. The best moment for application of Nd:YAG laser is after the use of adhesive system. Self-etching adhesive systems tested in this study can be used together with Nd:YAG laser without compromising to adhesion to dentine.