Related Experiment Video
Updated: Apr 12, 2026

Force System with Vertical V-Bends: A 3D In Vitro Assessment of Elastic and Rigid Rectangular Archwires
Published on: July 24, 2018
Effect of fluoride on nickel-titanium and stainless steel orthodontic archwires: an in-vitro study
Farzin Heravi1, Mohamad Hadi Moayed2, Nima Mokhber3
1Department of Orthodontics, School of Dentistry Mashad University of Medical Sciences, Mashhad, Iran.
Objectives:
The commonly used Nickel-Titanium (NiTi) archwires in orthodontic treatment are often exposed to fluoride-containing mouthwashes. The aim of this in-vitro study was to evaluate and compare the corrosion resistance of three commercially available NiTi archwires exposed to 0.05 wt% and 0.2 wt% fluoride mouthwashes.
Materials And Methods:
Three different types of NiTi archwires, 0.016″ in diameter, from Dentaurum, Global, and GAC, and a stainless steel archwire from Dentaurum were examined to assess their corrosion resistance in Fusayama-Meyer artificial saliva and in two other artificial saliva containing 0.05 wt% and 0.2 wt% sodium fluoride (NaF). After the primary setup of wires, they were tested by potentiodynamic and potentiostatic polarization and corrosion potential/time analyses. Their surfaces were evaluated using a scanning electronic microscope (SEM).
Results:
The results showed that all the wires were passive in artificial saliva. In contrast, by adding fluoride ions to the solution, the decrease in the archwires' corrosion resistance was in direct proportion to the increase in fluoride concentration.
Conclusion:
The NiTi wires experienced deterioration of their corrosion properties under the effect of fluoride but not as much as the stainless steel archwires.